RhythmLocks

Hair Make-Up (CPF 4435)

Why restrict the power of make-up to our faces? Using a film former for long-lasting, non-transfer neon colors, this hair make-up provides good styling performance while remaining easy to remove with shampoo.

RhythmLocks

Formulation:

Phase

Trade name / Supplier

INCI name

Wt. %

A

Water / Aqua

Water / Aqua

67.20

MaizeCare™ Style Polymer / Dow

Hydrolyzed Corn Starch

3.00

Phenoxyethanol Low Phenol / Clariant

Phenoxyethanol

0.90

B

Propylene Glycol

Propylene Glycol

1.50

ACULYN™ 88 Rheology Modifier / Dow

Acrylates / Steareth-20 Methacrylate Crosspolymer

3.00

Covarine White WN 9787 / Sensient

CI 77891 (and) Aqua (and) Glycerin (and) Xanthan Gum (and) Sodium Citrate

1.60

Covarine Red WS 3797 / Sensient

CI 12490 (and) Glycerin (and) Aqua (and) Sodium Laureth Sulfate (and) Diethylhexyl Sodium Sulfosuccinate

2.50

C

DOWSIL™ FA 4012 ID Silicone Acrylate / Dow

Isododecane (and) Acrylates / Polytrimethylsiloxymethacrylate Copolymer

5.00

Purolan IDD / Lanxess

Isododecane

7.00

DOWSIL™ 556 Cosmetic Grade Fluid / Dow

Phenyl Trimethicone

3.00

Tween 20 / Croda

Polysorbate 20

1.00

Eumulgin CO 40 / BASF

PEG-40 Hydrogenated Castor Oil

1.00

D

Colorona SynBerry Pink / Merck

Synthetic Fluorphlogopite (and) Titanium Dioxide (and) Carmine (and) Tin Oxide

0.60

Ballerina 187690 / Symrise

Fragrance

0.20

E

AMP Ultra PC 1000 (sol. 30%) / Angus

Aminomethyl Propanol

1.00

F

DOWSIL™ 969 Emulsion / Dow

Amodimethicone (and) Cetrimonium Chloride (and) Trideceth-3 (and) Trideceth-15

1.50

Disclaimer: Any variation in the formulation may cause performance to change.

Procedure:

  1. Sprinkle MaizeCare™ Style Polymer into the vortex of water heated at 70-80°C (water bath) at 400 rpm. Maintain heat and agitation until dispersion is complete (20-30 min).

  2. Once the dispersion is completed, add the phenoxyethanol under agitation.

  3. Remove from heat and add phase B ingredients to phase A one-by-one under mixing.

  4. Mix phase C ingredients together in a separate beaker.

  5. When phase AB is below 40°C, add phase C slowly under high shear (1000 rpm). Viscosity of formulation will increase slightly.

  6. Add phase D ingredients to phase ABC under normal mixing (400 rpm).

  7. Adjust pH of the formulation to 7 with phase E ingredient. Viscosity will increase drastically.

  8. Add phase F ingredient and stir until well incorporated (increase mixing speed if needed).